Low-alloy CrMnSi and CrNiMo steels, HB / HRC hardness values, the role of heat treatment and the balance between hardness and toughness.

Material

Bucket teeth are usually cast from low-alloy CrMnSi (25/30/35CrMnSi) or CrNiMo steel. The alloying elements determine hardenability and impact strength.

Balancing hardness and toughness

Typical tooth hardness is HRC 45 – 52 (about 430 – 520 HB). A harder tooth wears more slowly but becomes more brittle, so surface and core hardness are measured separately and toughness is checked with a Charpy impact test.

Heat treatment

After casting, quenching at 850 – 930 °C and tempering at 190 – 250 °C give the tooth both wear resistance and toughness.